Small batch production of plastic parts of silicone mould
requirements of small batch sample copy of the production.
Process:
Silicone mold preheating. The silicone mould is heated to 60-70, and the mold temperature is too low, it will cause the curing
is not complete, causing the physical properties of the poor. Die temperature has a direct relationship to the size accuracy of the test piece.
Castable pre deaeration. The A, B two liquid vacuum defoamation treatment for more than 30 minutes in the vacuum box.
Pouring. Will be filled with A liquid and B liquid containers were placed in the operating room. Working chamber pumped to
vacuum from time to time mixing solution B to deaeration 5-10 minutes, a liquid into liquid B in stirring 30-40 minutes after
quickly poured into the silicon rubber mold. And the operation of the 1 -1 in 30 seconds after the start of the mixing.
Solidification In the constant temperature box of 60-70 for 30-60 minutes after curing, you can release. 2-3 hours of the two
curing in the constant temperature box at 70-80 is necessary.